MIM STAINLESS STEELS

Materials Nominal
Composition
%
Density
*
Conditions Hardness Tensile
Strength
MPa(ksi)
Yield
Strength
MPa(ksi)
Elongation
AISI 430L
1.4016
X8Cr17
Cr:16.0-18.0; C:0.01 max
Ni:0.15 max; Mn:1.0 max
Si:1.0 max; S: 0.03 max
P:0.04 max; Fe: Balance
7.4 Sintered 69HRB 370 (54) 245 (36) 25
AISI 316L
1.4435 1.4404
X2CrNiMo17132
Cr:16.0-18.0;Ni:10.0-14.0
Mo:2.0-3.0; Si:1.0 max
Mn:2.0 max; C:0.01 max
Fe:Balance
7.6 Sintered 60HRB 482 (70) 164 (24) 55
AISI 304L
1.4306
X2CrNi1911
Cr:18.0-20.0; Ni:8.0-12.0
C:0.03 max; Mn:2.0 max;
P:0.045 max; S:0.03 max;
Si:1.0 max; Fe: Balance
7.5 Sintered 60HRB 495 (72) 160 (23) 50
AISI 17-4PH
1.4542
1.4548
X5CrNiCuNb174
Cr:15.5-17.5; Ni: 3.0-5.0
Cu:3.0-5.0; C:0.03 max
Nb+Ta:0.15 -0.45
Mn:1.0 max; Si:1.0 max
P:0.04 max.; Fe:Balance
7.65 Sintered
Heat Treated
20HRC
38HRC
824 (120)
1104 (160)
695 (101)
980 (142)
10
3
AISI 420
1.4021
X20Cr13
Cr:12.0-14.0; C:0.15 min
Mn:1.0 max; Si:1.0 max
Ni:0.35 max; P:0.04 max
S:0.03 max; Fe:Balance
7.45 Sintered
Heat Treated
103HRC
50HRC
1135 (165)
1400 (203)
690 (100)
1000 (145)
 
AISI 440C
1.4125
X105CrMo17
C:0.95-1.20; Cr:16.0-18.0
Si:1.0max; Mn:1.0max
S:0.03 max; Mo:0.75max
N:0.03max; P:0.045max
Ni:0.50max; O: 0.1 max
Fe:Balance
7.40
7.66
Sintered
Sintered+HIP
Heat Treated
690-740HV      
The given properties represent typical average values
*Pycnometric Density